Chemical Compositions
Exotic Nickel Alloys
| Grade | UNS No. | EN No. | C | Mn | Si | P | S | Cr | >Ni | Mo | Other |
|---|---|---|---|---|---|---|---|---|---|---|---|
| Nickel 200 | N02200 | 2.4066 | 0.01 | 0.35 | 0.35 | - | 0.01 | - | 99 | - | Cu: 0.25 |
| Nickel 201 | N02201 | 2.4068 | 0.02 | 0.35 | 0.35 | - | 0.01 | - | 99 | - | Cu: 0.25 |
| Monel 400 | N04400 | 2.4360 | 0.3 | 2 | 0.5 | - | 0.024 | - | 63 | - | Cu: 28-34 |
| Alloy 600 | N06600 | 2.4816 | 0.15 | 1 | 0.5 | - | 0.015 | 14-17 | 72 | - | Cu: 0.5 |
| Alloy 625 | N06625 | 2.4856 | 0.1 | 0.5 | 0.5 | 0.015 | 0.015 | 20-23 | 58 | 9 | - |
| Alloy 800 | N08800 | 1.4550 | 0.1 | 1.5 | 1 | - | 0.015 | 19-23.5 | 30-35 | - | Cu:0.75 |
| Alloy 800H | N08810 | 1.4876 | 0.05 - 0.1 | 1.5 | 1 | - | 0.015 | 19-23.5 | 30-35 | - | Cu:0.75 |
| Alloy 800HT | N06022 | 2.4602 | 0.01 | 0.5 | 0.08 | 0.02 | 0.02 | 20-22.50 | 12.5 - 14.5 | ||
| Alloy 20 | N08020 | 2.4660 | 0.07 | 2 | 1 | 0.045 | 0.035 | 19-21 | 32 - 38 | 2 - 3 | Cu: 3 - 4 |
| Alloy 825 | N08825 | 2.4858 | 0.05 | 1 | 0.5 | - | 0.03 | 19-23.5 | 38-46 | 2.5-3.5 | Cu: 1.5-3 |
| Alloy 28 | N08028 | 1.4563 | ≤ 2.5 | 26-28 | 30-34 | 3-4 | |||||
| Hastelloy C-22 | N06022 | 2.4602 | 0.015 max | 0.5 max | 0.08 max | 0.02 max | 0.02 max | 20-22.5 | 50.01-63 | 12.5-14.5 | |
| Hastelloy C276 | N10276 | 2.4819 | 0.01 | 1 | 0.08 | 0.04 | 0.03 | 14-16.5 | Rest | 15-17 |
Austenitic Stainless Steel
| Grade | UNS No. | EN No. | C | Mn | Si | P | S | Cr | Ni | Mo | Other |
|---|---|---|---|---|---|---|---|---|---|---|---|
| TP 304 | S30400 | 1.4301 | 0.07 | 2.00 | 1.00 | 0.045 | 0.015 - 2.00 | 17.50 - 19.50 | 8.00 - 10.50 | N: 0.11 | |
| TP 304L | S30403 | 1.4307 | 0.03 | 2.00 | 1.00 | 0.045 | 0.3 | 18.00 - 20.00 | 8.00 - 12.00 | N: 0.10 | |
| TP 304H | S30409 | 1.4948 | 0.04 - 0.08 | 2.00 | 1.00 | 0.035 | 0.015 - 2.00 | 17.00 - 19.00 | 8.00 - 11.00 | N: 0.11 | |
| TP 309 | S30900 | 1.4828 | 0.20 | 2.00 | 1.50 - 2.50 | 0.045 | 0.015 | 19.00 - 21.00 | 11.00 - 13.00 | N: 0.11 | |
| TP 310S | S31008 | 1.4845 | 0.10 | 2.00 | 1.50 | 0.045 | 0.015 | 24.00 - 26.00 | 19.00 - 22.00 | N: 0.11 | |
| TP 316 | S31600 | 1.4401 | 0.0 - 0.07 | 0.00 - 2.00 | 0.00 - 1.00 | 0.00 - 0.05 | 0.0 - 1.00 | 16.50 - 18.50 | 10.00 - 13.00 | 2.00 - 2.50 | N: 0.0 - 0.11 |
| TP 316L | S31603 | 1.4404 | 0.030 | 2.00 | 1.00 | 0.045 | 0.015 - 2.00 | 16.50 - 18.50 | 10.00 - 13.00 | 2.00 - 2.50 | N: 0.11 |
| TP 316H | S31609 | 1.4918 | 0.04 - 0.08 | 2.00 | 0.75 | 0.035 | 0.015 | 16.00 - 18.00 | 12.00 - 14.00 | 2.00 - 2.50 | N: 0.10 |
| TP 316 Ti | S31635 | 1.4571 | 0.08 | 2.00 | 1.00 | 0.045 | 0.015 - 2.00 | 16.50 - 18.50 | 10.50 - 13.50 | 2.00 - 2.50 | Ti: 5 x C to 0.70 |
| TP 317 | S31700 | 1.4449 | 0.08 | 2.00 | 1.00 | 0.045 | 0.3 | 19.00 | 13.00 | 3.5 | Fe: 61 |
| TP 317L | S21703 | 1.4438 | 0.030 | 2.00 | 1.00 | 0.045 | 0.015 - 2.00 | 17.50 - 19.50 | 13.00 - 16.00 | 3.00 - 4.00 | N: 0.11 |
| TP 321 | S32100 | 1.4541 | 0.08 | 2.00 | 1.00 | 0.045 | 0.015 - 2.00 | 17.00 - 19.00 | 9.00 - 12.00 | Ti: 5 x C to 0.70 | |
| TP 321H | S32109 | 1.4878 | 0.04 - 0.10 | 2.00 | 1.00 | 0.045 | 0.03 | 17.00 - 19.00 | 9.00 - 12.00 | Ti: 0.35 | |
| TP 347 | S34700 | 1.4550 | 0.08 | 2.00 | 1.00 | 0.045 | 0.015 | 17.00 - 19.00 | 9.00 - 12.00 | ||
| TP 347H | S34709 | 1.4961 | 0.04 - 0.10 | 2.00 | 1.00 | 0.040 | 0.03 | 17.00 - 20.00 | 9.00 - 13.00 | Fe: 62.83 - 73.64 | |
| TP 304L | S30403 | 1.4306 | 0.03 | 2.00 | 1.00 | 0.045 | 0.015 | 18.00 - 20.00 | 10.00 - 12.00 | N: 0.11 |
Super Austenitic Stainless Steel
| Grade | UNS No. | EN No. | C | Mn | Si | P | S | Cr | Ni | Mo | Other |
|---|---|---|---|---|---|---|---|---|---|---|---|
| 254 SMO | S31254 | 1.4541 | 0.020 | 1.00 | 0.70 | 0.030 | 0.010 | 19.50 - 20.50 | 17.50 - 18.50 | 6.00 - 7.00 | Cu: 0.50 - 1.00 |
| 904L | N08904 | 1.4539 | 0.020 | 2.00 | 0.70 | 0.030 | 0.010 | 19.00 - 21.00 | 24.00 - 26.00 | 4.00 - 5.00 | Cu: 1.20 - 2.00 |
| 253 MA | S30815 | 1.4835 | 0.05 - 0.12 | 1.00 | 1.40 - 2.50 | 0.045 | 0.015 | 20.00 - 22.00 | 10.00 - 12.00 | N: 0.12 - 0.20 | |
| 1.4435 | S31603 | 1.4435 | 0.030 | 2.00 | 1.00 | 0.045 | 0.015 - 2.00 | 17.00 - 19.00 | 12.50 - 15.00 | 2.50 - 3.00 | N: 0.11 |
| TP 310L NAG | S31002 | 1.4335 | 0.20 | 2.00 | 0.25 | 0.025 | 0.010 | 24.00 - 26.00 | 20.00 - 22.00 | 0.020 | N: 0.11 |
| TP 304 LN | S30453 | 1.4311 | 0.030 | 2.00 | 1.00 | 0.045 | 0.015 - 2.00 | 17.50 - 19.50 | 8.50 - 11.50 | N: 0.12 - 0.22 | |
| TP 314 | S31400 | 1.4811 | 0.20 | 2.00 | 1.50 - 2.50 | 0.045 | 0.015 | 24.00 - 26.00 | 19.00 - 22.00 | N: 0.11 | |
| TP 316 L N | S31653 | 1.4406 | 0.030 | 2.00 | 1.00 | 0.045 | 0.015 - 2.00 | 16.50 - 18.50 | 10.00 - 12.50 | 2.00 - 2.50 | N: 0.12 - 0.22 |
| TP 317 LMN | S31726 | 1.4439 | 0.030 | 2.00 | 1.00 | 0.045 | 0.015 | 16.50 - 18.50 | 12.50 - 14.50 | 4.00 - 5.00 | N: 0.12 - 0.22 |
Duplex & Super Duplex Stainless Steel
| Grade | UNS No. | EN No. | C | Mn | Si | P | S | Cr | Ni | Mo | Other |
|---|---|---|---|---|---|---|---|---|---|---|---|
| 2205 | S31803 | 1.4462 (6) | 0.030 | 2.00 | 1.00 | 0.035 | 0.015 | 21.00 - 23.00 | 4.50 - 6.50 | 2.50 - 3.50 | N: 0.12 - 0.22 |
| 2205 | S32205 | 1.4462 | 0.030 | 2.00 | 1.00 | 0.035 | 0.015 | 22.00 - 23.00 | 4.50 - 6.50 | 2.50 - 3.50 | N: 0.14 - 0.20 |
| 2304 | S32304 | 1.4362 | 0.030 | 2.00 | 1.00 | 0.035 | 0.015 | 22.00 - 24.00 | 3.50 - 5.50 | 0.10 - 0.60 | N: 0.05 - 0.20 |
| 2507 | S32750 | 1.4410 (9) | 0.030 | 2.00 | 1.00 | 0.035 | 0.015 | 24.00 - 26.00 | 6.00 - 8.00 | 3.00 - 4.50 | N: 0.24 - 0.35 |
| F55 | S32760 | 1.4501 | 0.030 | 1.00 | 1.00 | 0.035 | 0.015 | 24.00 - 26.00 | 6.00 - 8.00 | 3.00 - 4.00 | N: 0.20 - 0.30 |
Ferritic & Martensitic Steel
| Grade | UNS No. | EN No. | C | Mn | Si | P | S | Cr | Ni | Mo | Other |
|---|---|---|---|---|---|---|---|---|---|---|---|
| TP 405 | S40500 | 1.4002 | 0.08 | 1.00 | 1.00 | 0.040 | 0.015 - 2.00 | 12.00 - 14.00 | AI: 0.10 - 0.30 | ||
| TP 410 | S41000 | 1.4006 | 0.08 - 0.15 | 1.50 | 1.00 | 0.040 | 0.015 - 2.00 | 11.50 - 13.50 | 0.75 |